- productspecificaties
- Verpakkingen
- vraag offerte
Proper weldings are subject to the recommended heat treatment. The deposit is resistant to seawater, thin acids and scale resistant in air and oxidizing gases up to 950°C . The weld deposit can be tempered and also can sustain working temperatures up to 450° C. and will offer scale resistance up to much higher temperatures. Preheating is recommended at 150 - 350° C. depending on the thickness of the base metal. Similar base metals should be pre-heated at 300° C to 400° C.
1.4016, 1.4511, 1.4122
X6Cr17, X3CrNb17, X39CrMo17-1
UNS S43000
AISI 430
Cast steels, hardfacing pumps, shafts, seats, steam valves etc. Surfacing: unalloyed and low-alloyed steels
Heat Treatment |
RP0,2 (MPa) |
Rm (MPa) |
A5 (%) |
Hardness |
---|---|---|---|---|
As Welded | 700 | 1100 | 15 | 48 HRc |
720°C±15°C 2h | 230 HB |